How to Manufacture Laminated Copper Foil Flexible Busbar
Laminated copper foil flexible busbar is a high-current flexible conductive component for new energy industry. It is stacked with multiple layers of 0.05–0.3mm T2 high-purity copper foil. Two terminals are integrated by polymer diffusion welding, while the middle section remains bendable for flexible installation. With optional insulated sleeve or integral TPE injection, it replaces rigid copper bar and braided copper wire.
Issued by Xi’an Zipeng Technology
1. Raw Material Selection
Conductive Core (Main Material)
- Copper foil: T2 pure copper / C11000 oxygen-free copper, Cu ≥99.95%, 100% IACS conductivity
- Single foil thickness options: 0.05 mm, 0.1 mm, 0.2 mm, 0.3 mm, 0.5 mm
- Thinner foil = better flexibility; thicker foil = higher single-layer ampacity
- Calculate total cross-section:
Single foil area × layer countto match required current load
Auxiliary Materials
- Surface plating: Tin (standard anti-oxidation), Nickel (high salt spray), Silver (low contact resistance for high-current charging)
- Insulation materials: PVC heat shrink tube, XLPE, PI polyimide film, TPE integral injection (high voltage insulation)
- Cleaning chemicals: Alkaline degreaser, mild acid deoxidizer, DI water
Required Production Equipment
CNC laser cutting machine, ultrasonic cleaning tank, polymer diffusion welding machine, CNC drilling machine, electroplating line, heat shrink oven, bending jig, electrical test bench
2. Complete Standard Production Process
Step 1: Precision Cutting Copper Foil
- According to drawing dimensions (total length, width, welded terminal length, flexible section length), cut continuous copper foil rolls into single pieces via laser or servo die-cutting.
- Control edge burr ≤0.02 mm; burrs cause partial discharge and interlayer short risk.
- Sort foils by size and stack layer by layer to reach designed total thickness.
Step 2: Deep Surface Cleaning (Critical for Welding Quality)
Oil, copper oxide and dust on foil surfaces will lead to poor diffusion bonding & delamination after long vibration.
- Ultrasonic alkaline degreasing (40–60℃, 3–5 min): Remove machine oil and surface dirt
- Mild acid pickling: Strip copper oxide film to expose fresh pure copper surface
- 3-stage DI water rinsing + hot air full drying (no residual water spots)
- Stack cleaned foils neatly, clamp both ends to keep alignment flat
Step 3: Core Process – Polymer Diffusion Welding
Only weld the two terminal zones; the middle section remains loose multi-layer flexible foil for bending.
- Clamp stacked foil terminals between two welding molds
- Set process parameters (adjust by total stack thickness):
- Temperature: 500–620℃
- Pressure: 10–30 MPa
- Holding time: 10–60 seconds
- High current heating + constant pressure trigger copper atom interdiffusion between layers, forming monolithic solid copper terminals without gaps or voids
- Alternative welding for small batches: Ultrasonic welding, laser spot welding (diffusion welding is mainstream for high-reliability energy storage/EV products)
Step 4: Post-Welding Machining
- Cool down naturally then remove welding flash and edge burrs by grinding
- CNC drill mounting holes on terminals for bolt connection; tap threads if required
- Bend forming (follow design bending angle/radius; avoid cross-grain sharp bending to prevent foil fracture)
Step 5: Anti-Oxidation Surface Plating on Terminals
All contact surfaces must be plated to reduce contact resistance and anti-tarnish:
- Tin plating: General power cabinet, low-cost standard option, plating thickness 3–8 μm
- Nickel plating: Outdoor, humid, dust-prone equipment, anti-corrosion
- Silver plating: EV fast-charging, high-frequency inverter, ultra-low contact resistance
Xi'an Zipeng Technology provides full customized service including drawing design, sample testing, mass production and technical support. All products pass 100% electrical & mechanical inspection before delivery, complying with IATF16949 and RoHS standards.